Civil Engineering April 2021 | Vol 29 No 3
42 April 2021 Civil Engineering This also shows that using trapezoidal AEP such as FHWA is not appropriate in scenarios where the designer does not apply prestress to the system. CORROSION CONSIDERATIONS ON GROUTED ANCHOR SDAs AND HOLLOW BAR SOIL NAILS (HBSN) The following questions were asked to respondents: Do you ever use SDAs in permanent applications? This question was asked to establish how respondents consider corrosion of lateral support steel reinforcement. Corrosion is an important consideration in both passive (soil nail excavation) and active (stressed grouted anchor) solutions. Two participants indicated that they have never been faced with this problem. Two others indicated that they will use SDAs in a permanent application and three others stated they would not use these bars in permanent applications. For passive applications, EN14490 – Execution of special geotechnical works – Soil nailing, recommends assessing the global corrosion index using Table 5. If no information is available (typical to many projects), the worst relevant case shall be considered. Sacrificial thickness single corrosion protection (SCP) allowances can be made on soil nail cross sectional thickness, using Table 6, in accordance with the cor- rosion classification derived from Table 5. Guidance on minimum required grout cover for a required service life (excluding any coatings) are provided in Table 7. The authors’ main concern with sacrificial thickness allowances on SDA couplers are discussed further below. Table 5 does not consider atmospheric corrosion that could be a major contrib- uting factor to durability if a grouted anchor head or nail head is not sufficiently protected, especially in coastal regions in South Africa (Figure 7). ISO 14713-1:2009 provides guidance on expected life of various protections systems, such as hot- dip galvanising and zinc diffusion. Zinc diffusion of +/- 70 μm, typically applied to SDAs due to the shaving of galvanised coating during drilling, will be fully oxidised in around nine years (Category C5) in accordance with ISO 14713- 1:2009. Double corrosion protection, to prevent atmospheric corrosion, in these areas is therefore considered crucial for permanent soil nailed solutions (typically problematic over top 1.5 m to 2 m of bar) for both TB500 and SDA. Photos of corrosion at a temporary SDA nail’s head, that has been exposed after being in the ground for two years and an exposed SDA bolt-connection Table 5 General method to assess corrosiveness (EN14490) Criterion Features Weight A of Criterion Type of soil T exture – heavy, plastic, sticky impermeable, – clayey sand, – light, permeable, sandy, cohesionless Peat and bog/marshlands Industrial waste – clinker, cinders, coal – builder waste (plaster, bricks) Polluted liquids – wastewater, industrial – water containing de-icing salts 2 1 0 8 8 4 6 8 Resistivity (Ω.cm) p < 1 000 1 000 < p < 2 000 2 000 < p < 5 000 5 000 < p 5 3 2 0 Moisture content Water table – brackish water (variable and permanent) Water table – pure water (variable or permanent) Above water table – moist soil water content >20%) Above water table – dry soil (Water content <20%) 8 4 2 0 pH <4 4 to 5 5 to 6 >6 4 3 2 0 Global Index Sum of scoring for various criterion ( ∑ A ) Soil corrosiveness Classification Index Highly corrosive I 13 or greater (or no corrosivity test undertaken) Corrosive II 9 to 12 Average corrosive III 5 to 8 Slightly corrosive IV 4 or less Table 6 Sacrificial thickness allowance on soil nails Overall index I/ Classification Short-term (<18 months) Short-term (1.5 years to <30 years) Long term (30 years to <100 years) 4/IV 0 2 mm 4 mm 5 to 8/III 0 4 mm 8 mm 9 to 12/II 2 mm 8 mm plastic sheath/duct 13/I (or no corrosivity test undertaken) plastic sheath shall be provided Table 7 Minimum grout cover to metallic part of nail Soil corrosiveness Service life of structure (years) Grout cover 5 25 50 75 100 IV 10 mm 20 mm 25 mm 35 mm Special consideration required III 20 mm 30 mm 40 mm 50 mm II 30 mm 40 mm 50 mm 75 mm I (or no corrosivity test undertaken) n/a n/a n/a n/a n/a
Made with FlippingBook
RkJQdWJsaXNoZXIy MzE5NDI=